Heat capacities of RCoO3(s) (R = La, Nd, Sm Eu, Gd, Tb, Dy and Ho) by differential scanning calorimetry Patil, A.; Parida, S.; Dash, S.; Venugopal, V.; Thermochimica Acta 2007, 465, 25-29
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Large sample (1 g) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 130 | 56.9 |
| 220 | 97.4 |
| 230 | 99.9 |
| 240 | 103.3 |
| 250 | 105.5 |
| 260 | 107.4 |
| 270 | 110.2 |
| 280 | 112.0 |
| 290 | 113.7 |
| 298.15 | 122.5 |
| 300 | 122.6 |
| 140 | 62.0 |
| 325 | 124.8 |
| 350 | 128.4 |
| 375 | 131.0 |
| 400 | 133.9 |
| 425 | 137.7 |
| 450 | 142.3 |
| 475 | 146.9 |
| 500 | 150.8 |
| 525 | 153.5 |
| 550 | 154.7 |
| 150 | 69.3 |
| 575 | 154.6 |
| 600 | 153.6 |
| 625 | 151.9 |
| 650 | 150.2 |
| 675 | 148.7 |
| 700 | 147.7 |
| 725 | 146.7 |
| 750 | 146.2 |
| 775 | 146.0 |
| 800 | 145.9 |
| 160 | 73.8 |
| 825 | 146.2 |
| 850 | 147.6 |
| 170 | 79.9 |
| 180 | 83.6 |
| 190 | 87.1 |
| 200 | 91.9 |
| 210 | 94.7 |
27618; cobalt lanthanum oxide; 05407