Heat capacities of RCoO3(s) (R = La, Nd, Sm Eu, Gd, Tb, Dy and Ho) by differential scanning calorimetry Patil, A.; Parida, S.; Dash, S.; Venugopal, V.; Thermochimica Acta 2007, 465, 25-29
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Large sample (1 g) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 130 | 57.2 |
| 220 | 91.6 |
| 230 | 93.8 |
| 240 | 95.8 |
| 250 | 97.8 |
| 260 | 98.7 |
| 270 | 100.5 |
| 280 | 102.3 |
| 290 | 104.1 |
| 298.15 | 105.8 |
| 300 | 105.9 |
| 140 | 62.7 |
| 325 | 110.3 |
| 350 | 116.0 |
| 375 | 120.4 |
| 400 | 122.9 |
| 425 | 124.8 |
| 450 | 127.1 |
| 475 | 130.3 |
| 500 | 134.5 |
| 525 | 139.2 |
| 550 | 144.1 |
| 150 | 67.7 |
| 575 | 148.3 |
| 600 | 151.4 |
| 625 | 153.2 |
| 650 | 153.3 |
| 675 | 152.1 |
| 700 | 149.9 |
| 725 | 147.1 |
| 750 | 144.3 |
| 775 | 141.9 |
| 800 | 140.3 |
| 160 | 72.3 |
| 825 | 139.4 |
| 850 | 138.5 |
| 170 | 76.4 |
| 180 | 80.2 |
| 190 | 83.5 |
| 200 | 86.5 |
| 210 | 89.2 |
27619; cobalt(III) neodymium(III) oxide; 05408