Heat capacities of RCoO3(s) (R = La, Nd, Sm Eu, Gd, Tb, Dy and Ho) by differential scanning calorimetry Patil, A.; Parida, S.; Dash, S.; Venugopal, V.; Thermochimica Acta 2007, 465, 25-29
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Large sample (1 g) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 130 | 58.4 |
| 220 | 101.3 |
| 230 | 105.0 |
| 240 | 107.6 |
| 250 | 110.9 |
| 260 | 114.2 |
| 270 | 117.1 |
| 280 | 119.7 |
| 290 | 122.6 |
| 298.15 | 124.4 |
| 300 | 124.6 |
| 140 | 67.7 |
| 325 | 129.2 |
| 350 | 134.7 |
| 375 | 138.7 |
| 400 | 142.5 |
| 425 | 146.0 |
| 450 | 152.5 |
| 475 | 155.6 |
| 500 | 158.9 |
| 525 | 162.3 |
| 550 | 165.6 |
| 150 | 75.6 |
| 575 | 165.7 |
| 600 | 171.3 |
| 625 | 173.3 |
| 650 | 173.3 |
| 675 | 174.7 |
| 700 | 175.3 |
| 725 | 175.2 |
| 750 | 175.4 |
| 775 | 173.1 |
| 800 | 171.1 |
| 160 | 79.9 |
| 825 | 168.1 |
| 850 | 163.4 |
| 170 | 84.4 |
| 180 | 87.6 |
| 190 | 91.1 |
| 200 | 94.7 |
| 210 | 98.5 |