Heat capacities of RCoO3(s) (R = La, Nd, Sm Eu, Gd, Tb, Dy and Ho) by differential scanning calorimetry Patil, A.; Parida, S.; Dash, S.; Venugopal, V.; Thermochimica Acta 2007, 465, 25-29
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Large sample (1 g) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 130 | 56.9 |
| 220 | 97.5 |
| 230 | 100.1 |
| 240 | 102.5 |
| 250 | 104.8 |
| 260 | 107.4 |
| 270 | 109.8 |
| 280 | 112.0 |
| 290 | 114.1 |
| 298.15 | 116.1 |
| 300 | 116.7 |
| 140 | 67.3 |
| 325 | 121.5 |
| 350 | 125.5 |
| 375 | 127.0 |
| 400 | 129.8 |
| 425 | 131.9 |
| 450 | 133.5 |
| 475 | 134.2 |
| 500 | 135.7 |
| 525 | 136.6 |
| 550 | 137.9 |
| 150 | 72.9 |
| 575 | 140.1 |
| 600 | 142.9 |
| 625 | 145.3 |
| 650 | 148.7 |
| 675 | 152.2 |
| 700 | 156.4 |
| 725 | 159.5 |
| 750 | 162.4 |
| 775 | 164.7 |
| 800 | 167.9 |
| 160 | 77.1 |
| 825 | 170.8 |
| 850 | 173.4 |
| 170 | 81.4 |
| 180 | 84.5 |
| 190 | 87.6 |
| 200 | 90.7 |
| 210 | 93.8 |
27625; cobalt holmium oxide; 05414