Calorimetric study of AlNd2: Heat capacity. Standard Gibbs energy of formation Morishita, M.; Yamamoto, H.; Kodera, M.; Ikeda, K.; Miura, S.; Yamada, Y.; Thermochimica Acta 2011, 526, 90-98
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Relaxation calorimetry
- Phase(s): Crystal 1
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 40.99 | 60.15 |
| 48.45 | 49.74 |
| 49.52 | 50.16 |
| 50.58 | 50.55 |
| 52.53 | 52.08 |
| 56.82 | 54.57 |
| 61.12 | 57.06 |
| 65.42 | 59.25 |
| 69.71 | 60.87 |
| 74.02 | 61.59 |
| 78.32 | 61.14 |
| 42.06 | 51.75 |
| 82.63 | 62.19 |
| 86.92 | 63.57 |
| 91.22 | 64.8 |
| 95.53 | 65.88 |
| 99.82 | 66.87 |
| 104.1 | 67.74 |
| 108.4 | 68.49 |
| 112.7 | 69.18 |
| 117.0 | 69.78 |
| 121.3 | 70.29 |
| 43.12 | 48.15 |
| 125.6 | 70.77 |
| 129.9 | 71.22 |
| 134.2 | 71.61 |
| 138.5 | 71.97 |
| 142.8 | 72.33 |
| 147.1 | 72.63 |
| 151.4 | 72.87 |
| 155.6 | 73.23 |
| 159.9 | 73.56 |
| 164.2 | 73.89 |
| 43.93 | 48.69 |
| 168.5 | 74.19 |
| 172.8 | 74.49 |
| 177.0 | 74.76 |
| 181.3 | 75.03 |
| 185.6 | 75.3 |
| 189.9 | 75.54 |
| 194.2 | 75.75 |
| 198.5 | 75.96 |
| 202.8 | 76.17 |
| 207.1 | 76.38 |
| 44.19 | 49.47 |
| 211.4 | 76.56 |
| 215.7 | 76.71 |
| 220.0 | 76.89 |
| 224.3 | 77.01 |
| 228.6 | 77.16 |
| 232.9 | 77.28 |
| 237.2 | 77.4 |
| 241.5 | 77.49 |
| 245.8 | 77.61 |
| 250.0 | 77.67 |
| 45.25 | 48.33 |
| 254.3 | 77.76 |
| 258.6 | 77.85 |
| 262.9 | 77.91 |
| 267.2 | 78.0 |
| 271.5 | 78.06 |
| 275.8 | 78.18 |
| 280.1 | 78.27 |
| 284.4 | 78.39 |
| 288.7 | 78.54 |
| 293.0 | 78.75 |
| 46.32 | 48.81 |
| 297.3 | 78.96 |
| 301.6 | 79.26 |
| 301.7 | 79.26 |
| 47.38 | 49.26 |
| 48.23 | 49.62 |
28098; aluminum, compound with neodymium (1:2); 08487