Heat capacity, enthalpy and entropy of SrBi2O4 and Sr2Bi2O5 Leitner, J.; Sedmidubský, D.; Růžićka, K.; Svoboda, P.; Thermochimica Acta 2012, 531, 60-65
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Relaxation method
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 1.93 | 0.018 |
| 3.39 | 0.087 |
| 3.60 | 0.1 |
| 3.83 | 0.12 |
| 4.07 | 0.15 |
| 4.35 | 0.18 |
| 4.62 | 0.22 |
| 4.92 | 0.27 |
| 5.25 | 0.33 |
| 5.58 | 0.4 |
| 5.95 | 0.47 |
| 2.05 | 0.02 |
| 6.33 | 0.57 |
| 6.75 | 0.69 |
| 7.18 | 0.82 |
| 7.65 | 0.98 |
| 8.14 | 1.16 |
| 8.67 | 1.39 |
| 9.23 | 1.64 |
| 9.83 | 1.95 |
| 10.47 | 2.29 |
| 11.14 | 2.7 |
| 2.18 | 0.024 |
| 11.87 | 3.17 |
| 12.63 | 3.72 |
| 13.45 | 4.35 |
| 14.32 | 5.07 |
| 15.25 | 5.86 |
| 16.24 | 6.79 |
| 17.30 | 7.81 |
| 18.41 | 8.97 |
| 19.61 | 10.23 |
| 20.88 | 11.66 |
| 2.32 | 0.028 |
| 22.23 | 13.17 |
| 23.67 | 14.95 |
| 25.19 | 16.66 |
| 26.83 | 18.63 |
| 28.57 | 21.06 |
| 30.42 | 23.31 |
| 32.39 | 25.82 |
| 34.49 | 28.25 |
| 36.73 | 30.8 |
| 39.11 | 33.53 |
| 2.47 | 0.034 |
| 41.63 | 36.68 |
| 44.34 | 39.39 |
| 47.21 | 42.57 |
| 50.27 | 45.79 |
| 53.53 | 49.16 |
| 57.00 | 52.61 |
| 60.69 | 56.15 |
| 64.62 | 59.71 |
| 68.81 | 63.35 |
| 73.27 | 67.04 |
| 2.63 | 0.041 |
| 78.01 | 70.73 |
| 83.07 | 74.5 |
| 88.45 | 78.36 |
| 94.18 | 82.21 |
| 100.27 | 86.32 |
| 106.77 | 90.17 |
| 113.68 | 94.22 |
| 121.04 | 98.18 |
| 128.87 | 102.21 |
| 137.22 | 106.15 |
| 2.80 | 0.05 |
| 146.12 | 110.09 |
| 155.57 | 114.17 |
| 165.64 | 118.29 |
| 176.35 | 122.28 |
| 187.72 | 125.98 |
| 200.20 | 129.53 |
| 201.64 | 130.72 |
| 203.69 | 130.78 |
| 205.69 | 131.14 |
| 207.77 | 131.68 |
| 2.98 | 0.061 |
| 209.78 | 132.28 |
| 3.17 | 0.073 |
28132; bismuth strontium oxide (Bi2SrO4); 05548