Heat capacity, enthalpy and entropy of SrBi2O4 and Sr2Bi2O5 Leitner, J.; Sedmidubský, D.; Růžićka, K.; Svoboda, P.; Thermochimica Acta 2012, 531, 60-65
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Large sample (1 g) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 253.50 | 146.55 |
| 296.38 | 154.85 |
| 301.49 | 155.46 |
| 306.59 | 156.69 |
| 311.69 | 157.57 |
| 316.80 | 158.48 |
| 321.90 | 159.08 |
| 327.01 | 160.09 |
| 332.12 | 160.97 |
| 337.22 | 161.75 |
| 342.32 | 162.52 |
| 256.05 | 147.15 |
| 347.43 | 163.81 |
| 352.54 | 164.24 |
| 256.05 | 146.75 |
| 260.64 | 148.14 |
| 265.75 | 148.96 |
| 270.86 | 149.72 |
| 275.96 | 151.04 |
| 281.07 | 152.31 |
| 286.17 | 153.46 |
| 291.27 | 153.9 |
| 260.64 | 147.4 |
| 296.38 | 154.83 |
| 301.49 | 156.02 |
| 306.59 | 156.68 |
| 311.69 | 157.56 |
| 316.80 | 158.62 |
| 321.90 | 159.31 |
| 327.01 | 160.48 |
| 332.12 | 161.44 |
| 337.22 | 161.99 |
| 342.32 | 162.97 |
| 265.75 | 149.06 |
| 347.43 | 163.44 |
| 352.54 | 164.8 |
| 270.86 | 149.96 |
| 275.96 | 151.09 |
| 281.07 | 151.83 |
| 286.17 | 152.74 |
| 291.27 | 154.04 |
28132; bismuth strontium oxide (Bi2SrO4); 05548