Heat capacity, enthalpy and entropy of SrBi2O4 and Sr2Bi2O5 Leitner, J.; Sedmidubský, D.; Růžićka, K.; Svoboda, P.; Thermochimica Acta 2012, 531, 60-65
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Large sample (1 g) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 260.65 | 191.82 |
| 306.60 | 203.42 |
| 311.70 | 205.71 |
| 316.81 | 205.44 |
| 321.91 | 206.38 |
| 327.01 | 207.85 |
| 332.12 | 208.72 |
| 337.22 | 210.04 |
| 342.32 | 211.11 |
| 347.43 | 211.45 |
| 352.54 | 212.5 |
| 265.76 | 193.4 |
| 260.65 | 192.13 |
| 265.76 | 193.56 |
| 270.86 | 195.09 |
| 275.96 | 196.33 |
| 281.07 | 197.48 |
| 286.17 | 198.28 |
| 291.27 | 199.44 |
| 296.38 | 201.06 |
| 301.49 | 202.73 |
| 306.60 | 203.42 |
| 270.86 | 195.67 |
| 311.70 | 204.97 |
| 316.81 | 205.54 |
| 321.91 | 206.7 |
| 327.01 | 206.53 |
| 332.12 | 208.19 |
| 337.22 | 209.19 |
| 342.32 | 211.22 |
| 347.43 | 211.56 |
| 352.54 | 212.82 |
| 275.96 | 196.28 |
| 281.07 | 197.43 |
| 286.17 | 198.75 |
| 291.27 | 199.71 |
| 296.38 | 202.06 |
| 301.49 | 203.1 |
28133; bismuth strontium oxide (Bi2Sr2O5); 05549