Dielectric and thermal properties of cerium dioxide up to 1000°C and the effect of the porosity for microwave processing studies Hammoud, H.; Vaucher, S.; Valdivieso, F.; Thermochimica Acta 2015, 617, 83-89
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: Small sample (50 mg) DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 300 | 57.89941872 |
| 800 | 73.52744256 |
| 820 | 73.59628848 |
| 900 | 73.579077 |
| 920 | 73.52744256 |
| 1000 | 73.47580812 |
| 1000 | 73.44138516 |
| 1000 | 73.45859664 |
| 1100 | 73.51023108 |
| 1000 | 73.61349996 |
| 400 | 62.09901984 |
| 420 | 65.42083548 |
| 500 | 67.985346 |
| 520 | 69.93024324 |
| 600 | 71.3415846 |
| 620 | 72.32263896 |
| 700 | 72.95946372 |
| 720 | 73.33811628 |
28940; ceric oxide; 05296