Thermodynamic investigation of thorium and strontium substituted monazite solid-solution Rawat, D.; Phapale, S.; Mishra, R.; Dash, S.; Thermochimica Acta 2019, 674, 10-20
- Journal: Thermochimica Acta
- Sample Quantity(ies): Molar heat capacity at constant pressure
- Methodology: DSC
- Phase(s): Crystal
- Substances:
Data
| T (K) | Cp (J mol-1 K-1) |
| 313 | 56.9 |
| 403 | 63.0 |
| 413 | 63.6 |
| 423 | 64.0 |
| 433 | 64.5 |
| 443 | 64.9 |
| 453 | 65.4 |
| 463 | 65.8 |
| 473 | 66.2 |
| 483 | 66.6 |
| 493 | 66.9 |
| 323 | 57.7 |
| 503 | 67.3 |
| 513 | 67.6 |
| 523 | 68.0 |
| 533 | 68.3 |
| 543 | 68.6 |
| 553 | 68.9 |
| 563 | 69.2 |
| 573 | 69.5 |
| 583 | 69.8 |
| 593 | 70.1 |
| 333 | 58.6 |
| 603 | 70.4 |
| 613 | 70.6 |
| 623 | 70.9 |
| 633 | 71.2 |
| 643 | 71.4 |
| 653 | 71.7 |
| 663 | 71.9 |
| 673 | 72.2 |
| 683 | 72.4 |
| 693 | 72.7 |
| 343 | 59.3 |
| 703 | 72.9 |
| 713 | 73.1 |
| 723 | 73.4 |
| 733 | 73.6 |
| 743 | 73.8 |
| 753 | 74.1 |
| 763 | 74.3 |
| 773 | 74.5 |
| 783 | 74.7 |
| 793 | 74.9 |
| 353 | 60.0 |
| 800 | 75.1 |
| 363 | 60.7 |
| 373 | 61.4 |
| 383 | 61.9 |
| 393 | 62.5 |
29718; zirconium oxide; 05989